Necking in Metal Stamping
Necking in Metal Stamping: Process, Formulas, Coefficients, and Design Guide
-
What Is Necking in Metal Stamping?
Necking is a stamping operation in which the open end of a pre-drawn hollow part or a tubular blank is reduced in diameter. In short, necking is the process of narrowing the mouth of a drawn cup or tube to a smaller opening, typically to form a shoulder, a narrow mouth, or a sealed-end configuration that a subsequent operation can finish.As a secondary forming operation, necking is almost always performed after deep drawing or tube preparation. It allows the manufacturer to produce hollow components with a stepped diameter profile without adding a separate piece or a costly joining step. Necking is widely used for automotive components, aerosol cans, cartridge cases, battery housings, hose connectors, filters, and countless cylindrical parts that need a reduced end diameter.
At China Custom Stamping, we frequently combine necking with deep drawing and other forming stages to deliver net-shape hollow parts. If you are evaluating a part that requires a reduced mouth, this guide explains how the process works, how to size the blank, and how to avoid the most common failure — wrinkling.
-
Deformation Analysis of the Necking Process
Before calculating the blank, it is essential to understand what happens to the material during necking. The stress-and-strain state of the deformation zone is shown in Fig. 7-10 of the reference textbook.

During necking, the metal in the deformation zone is subjected to a tangential compressive stress σ₁ and an axial compressive stress σ₃. These two stresses produce:
- Elongation strains ε₃ and ε₂ in the axial and thickness directions; and
- A compressive strain ε₁ in the tangential (circumferential) direction.
Because the material is mainly under tangential compressive stress, the diameter decreases while the wall thickness and height increase. In practical terms, this means a necked part does not simply shrink — its wall thickens and its overall length grows slightly, which is why the blank-height formulas below include correction factors.
Why Wrinkling Happens
The same tangential compressive stress that shrinks the diameter is also the reason the necking process is prone to instability and wrinkling. Two zones are at risk:
- The deformation zone itself, which tends to buckle inward or wrinkle as the diameter is reduced under compression.
- The non-deformation zone (the barrel wall), which carries the entire necking force and can itself lose stability and deform.
Consequently, preventing instability is the main objective of the necking process. Choosing the right die support, controlling the cone angle, and staying within the limiting necking coefficient are the practical measures used to keep the process stable.
-
Necking Coefficient and Limiting Necking Coefficient
The degree of deformation in necking is expressed by the necking coefficient Ks:
Ks = d / d₀ (Eq. 7-13)
where:
- d — diameter of the part after necking, mm
- d₀ — diameter of the part before necking, mm
The maximum possible deformation is expressed by the limiting necking coefficient. Its value mainly depends on:
- The material properties (strength and ductility);
- The material thickness;
- The surface quality of the blank; and
- The shape of the necking die (especially whether internal or external support is provided).
Average Necking Coefficients of Various Materials (Table 7-8)
The table below gives the average necking coefficient Ksp for common materials under three die-support conditions:
|
Material
|
No Support
|
External Support
|
Internal Support
|
|
Soft steel
|
0.70 – 0.75
|
0.55 – 0.60
|
0.30 – 0.35
|
|
Brass
|
0.65 – 0.70
|
0.50 – 0.55
|
0.27 – 0.32
|
|
Aluminum
|
0.68 – 0.72
|
0.53 – 0.57
|
0.27 – 0.32
|
|
Hard aluminum (annealed)
|
0.75 – 0.80
|
0.60 – 0.63
|
0.35 – 0.40
|
|
Hard aluminum (quenched)
|
0.75 – 0.80
|
0.68 – 0.72
|
0.40 – 0.43
|
Notes:
- External support refers to clamping support on the outer diameter.
- Internal support refers to support provided by a mandrel inside the hole.
As the table shows, adding a mandrel (internal support) dramatically lowers the usable coefficient — meaning a much larger diameter reduction can be achieved in a single pass without wrinkling. External clamping also improves stability versus no support at all.
Effect of Material Thickness (Table 7-9)
Thicker material is more resistant to buckling, so the necking coefficient can be lower. The relationship is summarized below:
|
Material
|
< 0.5 mm
|
0.5 – 1 mm
|
> 1 mm
|
|
Brass
|
0.85
|
0.80 – 0.70
|
0.70 – 0.65
|
|
Soft steel
|
0.80
|
0.75
|
0.70 – 0.65
|
Multi-Pass Necking
When the required necking coefficient is smaller than the limiting value for the material, the part cannot be necked in a single operation and must go through multiple necking stages. In multi-pass necking:
- The first operation uses a coefficient about 10% smaller than the average value Ksp.
- Each subsequent operation uses a coefficient about 5% to 10% larger than the average.
This stepwise strategy lets the manufacturer reach a very small final diameter while keeping every individual pass stable.
-
Necking Process Calculation: Blank Size and Necking Force
Section 7.3.2 of the reference covers the calculation methods for the three most common necking forms, shown in Fig. 7-11: (a) tapered (conical), (b) straight, and (c) spherical.

4.1 Tapered (Conical) Neck — Blank Height (Eq. 7-14)
For the tapered necking form of Fig. 7-11(a), the blank height is:
h₀ = (1 ~ 1.05) · [ h₁ + (d₀² − d²) / (8·d₀·sinα) · (1 + √(d₀/d)) ] (Eq. 7-14)
4.2 Straight Neck — Blank Height (Eq. 7-15)
For the straight necking form of Fig. 7-11(b), the blank height is:
h₀ = (1 ~ 1.05) · [ h₁ + h₂·√(d/d₀) + (d₀² − d²) / (8·d₀·sinα) · (1 + √(d₀/d)) ] (Eq. 7-15)
4.3 Spherical Neck — Blank Height (Eq. 7-16)
For the spherical necking form of Fig. 7-11(c), the blank height is:
h₀ = h₁ + ¼ · (1 + √(d₀/d)) · √(d₀² − d²) (Eq. 7-16)
In Eqs. 7-14 through 7-16, d₀ and d are taken as the mid-diameter (the average of the outer and inner diameters). The factor (1 ~ 1.05) provides a small allowance so that the finished neck reaches the required height.
4.4 Selecting the Die Cone Half-Angle α
The half cone angle α of the necking die plays an important role in necking formation. In general, α should be kept within 30° so that the necking process proceeds favorably. A larger angle increases the tangential compressive stress and the risk of instability, while a smaller angle produces a longer, smoother transition zone.
4.5 Necking Force (Eq. 7-17)
For a tapered (conical) necked part formed with a die without internal support, the necking force is calculated as:
F = k · [ 1.1·π·d₀·t·σb · (1 − d/d₀) · (1 + μ·cotα) · (1 / cosα) ] (Eq. 7-17)
where:
- F — necking force, N
- k — coefficient; take 1.15 when using a press
- d₀ — diameter before necking, mm
- t — material thickness before necking, mm
- σb — tensile strength of the material, MPa
- d — diameter of the necked portion, mm
- μ — coefficient of friction between the part and the die
- α — cone half-angle of the die
This formula gives the force the press must deliver and is used to size the press tonnage and to verify the die and tooling stiffness.
-
Worked Example: Sizing a Tapered Neck
To show how the calculation is applied in practice, consider a soft-steel cup that is drawn to an outside diameter d₀ = 60 mm with a wall thickness t = 1.2 mm, and must be necked to a tapered opening with a final outside diameter d = 45 mm, a cone half-angle α = 20°, a straight cylindrical neck height h₁ = 10 mm, and a material tensile strength σb = 370 MPa.
Step 1 — Check the necking coefficient.
Ks = d / d₀ = 45 / 60 = 0.75
From Table 7-8, soft steel with no support allows a coefficient of 0.70–0.75, so a single pass is borderline acceptable without a mandrel. To be safe, an external clamp or a slightly larger first-pass diameter is recommended in production.
Step 2 — Estimate the blank height with Eq. 7-14 (using mid-diameters).
For a drawn part, the mid-diameter is roughly the outside diameter minus the wall thickness. Using d₀ ≈ 58.8 mm and d ≈ 43.8 mm, and sin 20° ≈ 0.342:
(d₀² − d²) / (8·d₀·sinα) = (3457.4 − 1918.4) / (8 × 58.8 × 0.342) = 1539 / 160.9 ≈ 9.6 mm
(1 + √(d₀/d)) = (1 + √(58.8/43.8)) = (1 + √1.343) = 1 + 1.159 ≈ 2.159
h₀ = 1.02 × [ 10 + 9.6 × 2.159 ] = 1.02 × [ 10 + 20.7 ] = 1.02 × 30.7 ≈ 31.3 mm
So the starting drawn cup should be roughly 31 mm tall before necking.
Step 3 — Estimate the necking force with Eq. 7-17.
With k = 1.15, μ = 0.10, and cot 20° ≈ 2.747, cos 20° ≈ 0.940:
F = 1.15 × [ 1.1 × π × 60 × 1.2 × 370 × (1 − 45/60) × (1 + 0.10 × 2.747) × (1 / 0.940) ]
= 1.15 × [ 1.1 × 3.1416 × 60 × 1.2 × 370 × 0.25 × 1.2747 × 1.0638 ]
Computing the bracket: 1.1 × 3.1416 ≈ 3.456; × 60 = 207.3; × 1.2 = 248.8; × 370 = 92,050; × 0.25 = 23,013; × 1.2747 = 29,335; × 1.0638 = 31,206 N.
F ≈ 1.15 × 31,206 ≈ 35,900 N ≈ 36 kN.
A press capable of roughly 5 tons or more is therefore appropriate for this part. This example is illustrative only — our engineers run these calculations per part and confirm them by tryout.
-
How to Design a Multi-Pass Necking Sequence
When a single pass is not possible, the sequence is planned step by step using the average coefficient Ksp as the reference. The working rule given in the reference is straightforward:
- Establish the final diameter d and the pre-neck diameter d₀, then compute the overall Ks = d/d₀.
- Compare Ks with the limiting coefficient for the material and the chosen support condition. If Ks is too small, plan several passes.
- First pass: use a coefficient about 10% smaller than Ksp. This deliberately takes a slightly more aggressive reduction first, when the material is still in its most formable state and the wall is thickest.
- Each subsequent pass: use a coefficient about 5% to 10% larger than Ksp. The later passes are progressively lighter because the wall has thinned and the part has already been work-hardened by the earlier reductions.
- Between passes, the intermediate geometry is re-calculated with the blank-height formulas so the transition zones line up and no pass introduces unnecessary strain.
Multi-pass necking is routine for deep-reduction parts such as gas cylinders, battery cans, and aerosol bodies. The extra tooling cost is offset by the ability to reach small final diameters without wrinkling or tearing.
-
Necking Die Construction and Support Options
The die design determines how much reduction is achievable. The three support conditions that appear in Table 7-8 correspond to three basic tooling arrangements:
- No support. The open cup is pushed into a conical die with nothing holding the outside or inside. Simple and inexpensive, but only suitable for mild reductions (higher coefficient).
- External support (outer-diameter clamping). A clamp or sleeve grips the outer diameter of the cup wall while the neck is formed. This restrains the non-deformation zone, preventing the barrel wall from buckling, and lowers the usable coefficient to the mid-range values in the table.
- Internal support (mandrel). A mandrel is inserted into the bore so the inner surface is supported during forming. This is the most stable arrangement and gives the lowest coefficients (0.27–0.43), enabling the deepest single-pass reductions.
Selecting the right support is therefore the single most influential decision in necking tooling. For thin-walled or high-ductility parts, internal support is usually preferred; for larger-diameter thick-walled parts, external clamping is often enough.
-
Design Guidelines for Reliable Necking
Based on the process fundamentals above, here are the practical rules we apply when designing necking tooling:
- Always check the necking coefficient first. If Ks = d/d₀ falls below the limiting value for your material and thickness, plan for multi-pass necking rather than forcing a single reduction.
- Use internal support (mandrel) when you need a large reduction. Table 7-8 shows internal support can lower the usable coefficient from about 0.7 down to about 0.3 — the difference between one pass and several.
- Keep the die half cone angle α within 30°. This directly controls wrinkling and forming stability.
- Account for wall thickening and length growth. Because necking thickens the wall and increases height, apply the (1 ~ 1.05) allowance in the blank-height formulas.
- Use the mid-diameter for d₀ and d in the blank-size equations, not the outer diameter.
- Size the press from the necking-force formula (Eq. 7-17) and add the coefficient k = 1.15 when using a press, so the chosen machine has adequate margin.
- Protect the non-deformation zone. Since the barrel wall carries the entire necking force, provide adequate guidance and support to prevent the wall from buckling.
- Control lubrication. Friction between the part and the die (μ) directly enters the force formula, so consistent lubrication keeps the process stable and the force predictable.
-
Common Defects in Necking and How to Avoid Them
Because necking is a compressive forming operation, the most frequent quality problems all trace back to instability:
- Wrinkling of the neck — caused by exceeding the limiting necking coefficient. Solution: reduce the reduction per pass, add a mandrel, or lower the cone angle.
- Buckling of the barrel wall — caused by inadequate support of the non-deformation zone. Solution: external clamping or better die guidance.
- Neck tearing or cracking — usually related to low-ductility material or a too-sharp transition. Solution: increase the cone angle within the 30° limit, or use a more formable material grade.
- Inconsistent neck height — caused by an under-sized blank or unstable blank holding. Solution: apply the (1 ~ 1.05) allowance and verify the blank height with Eqs. 7-14 to 7-16.
Early verification of the necking coefficient is the most effective way to prevent these defects before any tool steel is cut.
-
Necking vs. Other Forming Operations
Necking is often confused with similar operations, so it helps to distinguish them:
- Necking reduces the open-end diameter of a drawn cup or tube under compressive stress.
- Ironing reduces wall thickness by passing the part through a smaller die.
- Flanging bends material outward to form a lip or collar.
- Curling rolls the edge into a rounded bead.
- Deep drawing forms the initial cup or shell that necking later modifies.
Because necking is a compressive forming operation, it is fundamentally different from operations that remove or bend material. This is why the coefficient-based calculation method is so important: it tells the tooling engineer, before any steel is cut, whether the part can be formed in one pass.
-
Applications of Necked Parts
Necking appears in nearly every industry that uses hollow metal components:
- Automotive: filler necks, hose connectors, shock-absorber tubes, exhaust transition pieces.
- Consumer goods: aerosol cans, spray bottles, bottle caps, can bodies.
- Industrial: pressure vessels, filter housings, hydraulic components, pipe fittings.
- Electronics and energy: battery cans, capacitor housings, and other drawn shells with reduced mouths.
In each case, necking lets a single drawn part do the work of several joined pieces, saving material, weight, and assembly cost.
-
Material Selection and Surface Quality
The limiting necking coefficient depends heavily on the material, and the tables in this guide reflect that dependency:
- Soft steel is the most forgiving of the common materials, offering a reasonable balance of strength and ductility. For a given thickness it tolerates a lower coefficient than brass or aluminum.
- Brass forms well but is more sensitive to work-hardening, so multi-pass sequences must step more carefully.
- Aluminum is light and ductile but prone to surface scoring and wrinkling at higher reductions; lubrication and die finish matter more.
- Hard aluminum behaves differently depending on its temper. The annealed grade allows a notably lower coefficient (0.35–0.40 with internal support), while the quenched grade (0.40–0.43) is harder and requires more support.
In addition to the alloy and temper, the surface quality of the blank directly influences the usable coefficient. A clean, well-lubricated, burr-free blank reduces friction (μ) and keeps the force and strain predictable. Scale, dirt, or heavy die pickup can raise friction enough to push an otherwise stable process into wrinkling or tearing. This is why blank preparation and die maintenance are treated as part of the process design, not as afterthoughts.
-
Inspection and Quality Control of Necked Parts
Because necking is a compressive process, the typical inspection points are different from those of a cutting or bending operation:
- Diameter and taper: verify d at the mouth and the transition geometry against the drawing, usually with a caliper or profile projector.
- Neck height: confirm h₀ matches the target, accounting for the slight height growth that the process introduces.
- Wall thickness: check that the neck wall has thickened as predicted and remains within the minimum-wall requirement.
- Surface condition: inspect for wrinkles, scoring, or micro-cracks at the transition radius.
- Force and process stability: during tryout, compare the measured press load with the value from Eq. 7-17 to confirm the die, lubrication, and support are performing as designed.
At our facility, these checks are performed on the first article and at agreed intervals during production, so the process stays in control across the full batch.
-
Partner With China Custom Stamping
Necking is just one of the forming techniques we use to produce precision hollow metal parts. From deep-drawn shells to necked and threaded components, our engineers size the blank, select the correct die support, and validate the press tonnage before production begins — so you get a stable, repeatable process and parts that meet your print.
Send us your drawing and target diameter; we will calculate the necking coefficient, recommend a single- or multi-pass approach, and provide a tooling and production quotation.
Related resources on our site: